GEN 276 Overview
GEN 276 is used for welding of materials of similar chemical composition (UNS Number N10276), as well as dissimilar materials of nickel base alloys, steels and stainless steels. This wire also can be used for cladding steel with nickel-chromium-molybdenum weld metal. This alloy, due to its high molybdenum content, offers excellent resistance to stress corrosion cracking, pitting, and crevice corrosion.
AWS 化学成分(典型)
| %C | %Cr | %Ni | %Mo | %W | %Fe | %Mn |
|---|---|---|---|---|---|---|
| 0.02 max 0.005 |
14.5 – 16.5 15.8 |
rem. 58.3 |
15.0 – 17.0 15.9 |
3.0 – 4.5 3.5 |
4.0 – 7.0 5.7 |
1.0 max 0.5 |
| %Si | %P | %S | %Cu | %Co | %V | 其他合计 |
|---|---|---|---|---|---|---|
| 0.08 max 0.05 |
0.04 max 0.005 |
0.03 max 0.001 |
0.50 max 0.1 |
2.5 max 0.2 |
0.35 max 0.03 |
0.50 max |
典型的焊接金属机械性能
| 抗拉强度 | 105,000 psi | 724 MPa |
| 屈服强度 | 80,000 psi | 551 MPa |
| 伸长 | 36% |
Typical Welding Parameters
| 过程 | Diameter | Voltage | Amperage | Gas/Flux |
|---|---|---|---|---|
| 氩弧焊 (GTAW) | 1/16” (1.6 mm) | 14 – 18 | 90 – 130 | 100% Ar |
| 3/32” (2.4 mm) | 15 – 20 | 120 – 175 | 100% Ar | |
| 1/8” (3.2 mm) | 15 – 20 | 150 – 220 | 100% Ar | |
| 米格 (GMAW) | .035” (0.9 mm) | 26 – 29 | 150 – 200 | 75% Ar – 25% He |
| .045” (1.1 mm) | 28 – 32 | 180 – 220 | 75% Ar – 25% He | |
| Sub Arc (SAW) | .093” (2.4 mm) | 28 – 31 | 300 – 350 | |
| .125” (3.2 mm) | 29 – 33 | 300 – 350 |