    CWI Generation4™ Stainless Steel and Nickel Welding wire alloys can be used with many different joint styles and welding processes. Once the weld joint style, the filler material, and the process has been identified, a proper welding procedure can be identified. The welding procedure chosen for Stainless Steel and Nickel welding depends upon the process to be used as well as the size and alloy of the actual consumable. The charts below provide detailed information on the voltage, amperage (current), and gas (atmosphere) to be used in TIG (Tungsten Inert Gas), MIG (Metal Inert Gas), and SAW (Submerged-Arc Welding) welding processed for the general alloys that we provide. If you have questions about selecting the right procedure, or about the recommended welding procedure for a specific CWI Generation4 ™ wire, contact a CWI material and applications expert today.
    Recommended Welding Procedures for Stainless Steel Welding Wire

    Recommended Welding Procedures for Gen 4 Stainless Steel Welding Wire

    ProcessDiameter of WireVoltage (V)Amperage (A)Gas
    TIG0.035"0.9 mm12-1560-90100% Argon
    0.045"1.1 mm13-1680-110100% Argon
    1/16"1.6 mm14-1890-130100% Argon
    3/32"2.4 mm15-20120-175100% Argon
    1/8"3.2 mm15-20150-220100% Argon
    MIG0.030"0.8mm24-28140-18099% Argon + 1% Oxygen -or- 97% Argon + 3% CO2
    0.035"0.9mm26-29160-21099% Argon + 1% Oxygen -or- 97% Argon + 3% CO2
    0.045"1.1mm28-32180-25099% Argon + 1% Oxygen -or- 97% Argon + 3% CO2
    SAW0.0625"1.6mm29-33200-280Suitable Flux may be used
    3/32"2.4mm28-30275-350Suitable Flux may be used
    1/8"3.2mm29-32350-450Suitable Flux may be used
    5/32"4.0mm30-33450-550Suitable Flux may be used
    Recommended Welding Procedures for Nickel Alloy Welding Wire

    Recommended Welding Procedures for Gen 4 Stainless Nickel Welding Wire

    ProcessDiameter of WireVoltage (V)Amperage (A)Gas
    TIG0.035"0.9 mm12-1560-90100% Argon
    0.045"1.1 mm13-1680-110100% Argon
    1/16"1.6 mm14-1890-130100% Argon
    3/32"2.4 mm15-20120-175100% Argon
    1/8"3.2 mm15-20150-220100% Argon
    MIG0.035"0.9mm26-29150-19075% Argon + 25% Helium
    0.045"1.2mm28-32180-22075% Argon + 25% Helium
    1/16"1.6mm29-33200-25075% Argon + 25% Helium
    SAW3/32"2.4mm28-30375-350Suitable Flux may be used
    1/8"3.2mm29-32350-450Suitable Flux may be used
    5/32"4.0mm30-33400-550Suitable Flux may be used