  • GEN 413

    GEN 413 Overview

    GEN 413 is used for welding 70‐30, 80‐20 and 90‐10 copper nickel alloys. It can also be used for dissimilar
    joining applications such as copper‐nickel alloys to nickel alloys. GEN 413 is occasionally used for overlay on
    carbon steel after applying a layer of ERNi‐1.

    Welding Wire Reels

    AWS Chemical Composition (Typical)

    %Ni %Cu %Fe %Pb %Mn
    29.0 – 32.0
    30.91
    Rem.
    67.2
    0.40 – 0.75
    0.55
    0.02 max
    0.005
    1.0 max
    0.78
    %Si %P %Ti Total Others
    0.25 max
    0.025
    0.02 max
    0.0015
    0.20 – 0.50
    0.40
    0.50 max

    Typical Weld Metal Mechanical Properties

    Tensile Strength 52,500 psi 362 MPa
    Yield Strength 21,000 psi 145 MPa
    Elongation (min.) 30%

    Typical Welding Parameters

    ProcessDiameterVoltageAmperageGas/Flux
    TIG (GTAW)1/16” (1.6 mm)14 – 1890 – 130100% Ar
    3/32” (2.4 mm)15 – 20125 – 175100% Ar
    1/8” (3.2 mm)15 – 20150 – 220 
    MIG (GMAW).035” (0.9 mm)26 – 29150 – 19098% Ar – 2% O2
    .045” (1.1 mm)28 – 32180 – 22098% Ar – 2% O2
    Sub Arc (SAW).093” (2.4 mm)28 – 30275 – 350 
    .125” (3.2 mm)29 – 32350 – 450 